样品在模拟液中浸泡7天,样品腐蚀。合金会产生白色腐蚀物质,铁会生锈。样品表面和模拟液中都会有。这些腐蚀物质是用水冲洗加稀酸消解完上icp,还是用水冲洗过滤腐蚀物质?
该帖子作者被版主 tang5662积分, 2经验,加分理由:话题
为您推荐
您可能想找: ICP-AES/ICP-OES 询底价
专属顾问快速对接
立即提交
liang1026
结帖率:
100%
关注:0 |粉丝:0
新手级: 新兵
liang1026
结帖率:
100%
关注:0 |粉丝:0
新手级: 新兵
EN 1811:2011+A1:2015 (E)
P12
8.2 Release procedure
......
After (168 ± 2) h, slowly remove the sample from the release solution. To collect solution contained in cavities
of the sample, the sample shall be turned appropriately. The sample shall not be rinsed.
该帖子作者被版主 tang5662积分, 2经验,加分理由:分享
zz125
结帖率:
100%
关注:0 |粉丝:0
新手级: 新兵
原文由 liang1026(liang1026) 发表:
EN 1811:2011+A1:2015 (E)
P12
8.2 Release procedure
......
After (168 ± 2) h, slowly remove the sample from the release solution. To collect solution contained in cavities
of the sample, the sample shall be turned appropriately. The sample shall not be rinsed.测试后的溶液浑怎么处理



liang1026
结帖率:
100%
关注:0 |粉丝:0
新手级: 新兵
zz125
结帖率:
100%
关注:0 |粉丝:0
新手级: 新兵
原文由 liang1026(liang1026) 发表:
针筒+滤膜,过滤。
不需要将那些腐蚀物质消解的咯  按照  将样品取出 加稀酸稳定镍再用针筒+滤膜过滤  不需要将那些腐蚀的沉积物消解的吧
liang1026
结帖率:
100%
关注:0 |粉丝:0
新手级: 新兵
浸泡168h后,转移液体,用稀硝酸定容至刻度(保持1%的硝酸浓度)。
不是太浑浊的话需要过滤。
liang1026
结帖率:
100%
关注:0 |粉丝:0
新手级: 新兵
浸泡168h后,转移液体,用稀硝酸定容至刻度(保持1%的硝酸浓度)。
不是太浑浊的话不需要过滤。
zz125
结帖率:
100%
关注:0 |粉丝:0
新手级: 新兵
原文由 liang1026(liang1026) 发表:
浸泡168h后,转移液体,用稀硝酸定容至刻度(保持1%的硝酸浓度)。
不是太浑浊的话不需要过滤。


谢谢
zz125
结帖率:
100%
关注:0 |粉丝:0
新手级: 新兵
原文由 zz125(v3137606) 发表:
谢谢
欧洲REACH法规
按照REACH法规((EC) No. 1907/2006)附录十七27点对镍释放的要求:
1) 皮肤长期直接接触的部件,小于0.5微克每平方厘米每周;
2) 耳朵和其它身体穿刺部件,小于0.2微克每平方厘米每周
修正案:EN 1811:2011 + A1: 2015
该修正案保持测量不确定度的概念,但修订了合格评定的解释。
根据9.22章,由于46%的测量不确定度,产品镍释放量大于或等于0.88微克每平方厘米每周为不合格,因此产品镍释放量小于0.88微克每平方厘米每周是被接受并允许投放到市场上的。(针对耳朵和其它身体穿刺部件是小于0.35微克每平方厘米每周)    那我们测试结果是0.77微克每平方厘米每周  按照reach是给不合格还是 根据46%的测量不确定度给合格??